Hairline Cracks in New Concrete: Plastic Shrinkage, Crazing and What Is Normal

Broom-finished concrete with scored control joints in Eastern Idaho by Skinner Customs

Written by

in

You walk out the morning after your new patio or driveway was poured, coffee in hand, and there they are. Thin little lines in the surface that were not there when the crew left. Some are short and run side by side. Some look like a spider web if you get down close.

Your stomach drops. Did they just pour you a bad slab?

Maybe, maybe not. I run Skinner Customs out of Rigby, and hairline cracks in new concrete are one of the most common calls I get from homeowners who had somebody else pour their slab. Most of the time the cracks are one of two things: plastic shrinkage cracks or crazing. Both are surface problems. Both are mostly preventable. Neither one usually means your slab is going to fall apart. But they tell you a lot about how the pour was run.

Two kinds of early cracks

Before anything else, it helps to know which one you are looking at. They look different, they show up at different times, and they come from different mistakes.

Plastic shrinkage cracks form while the concrete is still soft, in the first few hours. They tend to run roughly parallel to each other, a foot or more apart, and they usually stop short of the edge of the slab.

Crazing is a fine web of very shallow cracks across the surface, like the glaze on an old plate. It usually shows up the day after the pour or within the first week, and it is easiest to see when the slab is drying after rain or a hose-down.

Real structural cracks that run the full depth of the slab, or cracks that have one side higher than the other, are a different conversation. I cover those in other posts on this blog. This one is about the surface.

Plastic shrinkage cracks: when the top dries too fast

The National Ready Mixed Concrete Association has a short technical bulletin on exactly this, CIP 5, Plastic Shrinkage Cracking. Here is how they describe what you are seeing:

“Plastic shrinkage cracks appear in the surface of fresh concrete soon after it is placed and while it is still plastic.”

And here is the cause, in one sentence:

“The critical condition exists when the rate of evaporation of surface moisture exceeds the rate at which rising bleed water can replace it.”

Fresh concrete is always pushing a little water up to the surface. That is called bleed water. As long as that water keeps up with what the sun and wind are pulling off the top, the surface stays wet and nothing happens. When the air pulls water off faster than the slab can replace it, the top layer shrinks while the concrete underneath has not, and it tears.

NRMCA lists the conditions that drive evaporation up:

  • Wind velocity in excess of 5 mph
  • Low relative humidity
  • High ambient and/or concrete temperatures

Read that list again and think about a summer afternoon in Eastern Idaho. Dry air, strong sun at elevation, and wind coming across the Snake River Plain most afternoons. We check all three boxes more days than not. That is why plastic shrinkage is something I plan for on every summer pour, not something I react to.

The good news, from the same bulletin:

“Plastic shrinkage cracks are unsightly but rarely impair the strength of concrete floors and pavements.”

The caution is that they are open doors. NRMCA notes they can let in aggressive chemicals and act as weak points where later cracking starts. On a driveway that is going to see snowmelt and road brine, that matters.

How a good crew prevents plastic shrinkage cracks

None of this is exotic. It is planning and having enough hands on site. These are the measures NRMCA lays out, and what they look like on a real job:

  1. Watch the forecast before the truck is ordered. If the afternoon is going to be hot, dry and windy, that changes the plan. Sometimes that means an earlier start. NRMCA also suggests windbreaks and sunshades when conditions are bad.
  2. Dampen a dry base. On a hot day a bone-dry gravel base will suck water out of the bottom of the slab. NRMCA says to dampen the subgrade “but not to a point that there is freestanding water prior to placement.”
  3. Keep the surface from drying between finishing steps. Evaporation retarders, fog spray, or covering the slab if there is a delay. A crew that is short-handed and falling behind is a crew that lets the surface dry out.
  4. Start curing right away. NRMCA calls for curing compound or wet covering as soon as possible, kept continuously moist for a minimum of 3 days.

One more item on their list is synthetic fibers in the mix. Some contractors use them for surface cracking. Fibers are not a substitute for steel. Every slab I pour gets rebar, and the surface-crack prevention comes from how the pour and cure are run.

Crazing: too much paste at the top

Crazing comes from a different direction. NRMCA covers it in CIP 3, Crazing Concrete Surfaces:

“Crazing is the development of a network of fine random cracks or fissures on the surface of concrete or mortar caused by shrinkage of the surface layer that is rich in paste or mortar.”

The cracks are shallow, rarely more than an eighth of an inch deep according to the bulletin, and the little cells between them are usually an inch and a half across or smaller. NRMCA is clear that they are not structural:

“They do not affect the structural integrity of concrete.”

So where does that paste-rich top layer come from? Almost always from the finishing. The bulletin lists the usual causes, and they read like a list of shortcuts:

  • Adding extra water at the truck to make the concrete easier to spread
  • Over-working the surface and driving the rock down
  • Finishing while bleed water is still on the surface
  • Sprinkling dry cement on the slab to soak up bleed water
  • Spraying water on the surface to make it easier to finish
  • Late or missing curing

Every one of those makes the top eighth of an inch weaker and richer in fine material than the rest of the slab. That layer shrinks more as it dries, and it crazes.

If you read my post on adding water to the truck, this will sound familiar. It is the same mistake showing up in a different way.

How crazing is prevented

NRMCA’s prevention list is the flip side of the cause list. Place concrete at a moderate slump instead of soupy. Do not finish while there is water on the surface. Never throw dry cement on a wet slab. Do not spray water to help the finish. Start curing as soon as finishing is done, and avoid letting the surface go through wet and dry swings in the first days.

Our exterior slabs get a broom finish as the standard, which helps here too. A broom finish leaves an open, textured surface instead of a slick, tight one, and the bulletin notes crazing is more noticeable on steel-troweled surfaces. Add a 4,000 PSI mix, a compacted gravel base, rebar and a real cure, and crazing becomes rare.

What to do if your new slab already has them

If the slab is already poured and you are seeing lines, here is how I would sort it out:

  • A web of tiny, shallow cracks you can barely catch a fingernail in: that is crazing. It is cosmetic. It may get more visible as dirt settles into it. Keep de-icers off it the first winter and a breathable sealer down the road can help keep water out.
  • A few straight cracks running roughly parallel, formed the first day: that is likely plastic shrinkage. Usually not a strength issue, but worth sealing so water and salt stay out.
  • Cracks that are wide, growing, cross the whole slab, or have one side higher than the other: that is not a surface issue. Get somebody to look at it.

Either way, take photos with a coin or a tape measure in the frame and note the date. If the cracks change, you want a record.

Frequently Asked Questions

Are hairline cracks in new concrete normal?

Some cracking in concrete is normal, which is why we cut control joints. Hairline surface cracks in the first day or week are usually plastic shrinkage or crazing. They are common, mostly cosmetic, and mostly preventable with good timing, finishing and curing.

Do plastic shrinkage cracks weaken the slab?

According to NRMCA, they “rarely impair the strength” of floors and pavements. They can let water and chemicals into the surface and become starting points for later cracks, so sealing them on an exterior slab is a good idea.

Is crazing a structural problem?

No. NRMCA’s bulletin says crazing does not affect the structural integrity of concrete. It is a weak, paste-rich surface layer that shrank as it dried. It is mostly a looks issue.

Can hairline cracks be fixed?

Plastic shrinkage cracks that open during finishing can sometimes be closed by refinishing on the spot. Once the slab has hardened, the practical step is keeping water out with a breathable sealer. You will not make them disappear.

What causes cracks the day after concrete is poured?

Usually the surface dried faster than the slab could replace the water, or too much water and paste ended up at the top from the mix or the finishing. Wind, low humidity, heat, extra water at the truck and late curing are the most common culprits.

When is it too windy to pour concrete?

There is no single cutoff, but NRMCA lists wind over 5 mph as one of the conditions that raise evaporation. On a dry, hot, windy day a good crew adjusts the start time, uses windbreaks or evaporation retarders, and has enough people to finish and cure fast.

Seeing lines in your new slab?

If you are in Rigby, Idaho Falls, Rexburg, Ammon or Shelley and you have a new slab with cracks you are not sure about, or you are planning a pour for spring and want it done right the first time, call me and I will tell you straight what you are looking at.

Need concrete work in Eastern Idaho? Call Zach at Skinner Customs at (208) 390-5794 or start at skinner-customs.com.


Content produced in partnership with S4 Media, marketing partner of SwagerBuilds LLC.

Comments

Leave a Reply

Your email address will not be published. Required fields are marked *