A few weeks after a new shop or garage floor goes in, the owner notices small bumps on the surface. Some are the size of a dime, some the size of a coaster. Then one cracks open under a tire and there is a hollow pocket under a thin skin of concrete. Or there are no bumps at all, but a section of the floor sounds different when you drop a wrench on it. Dull. Hollow.
That is blistering and delamination. I run Skinner Customs out of Rigby, and while these two problems are less common than cracks or scaling, they are some of the most frustrating, because the slab looked perfect on pour day. The cause is almost always timing during finishing, and it is very preventable.
What concrete blisters are
The National Ready Mixed Concrete Association explains this in CIP 13, Blisters on Concrete Slabs:
“Blisters are hollow, low-profile bumps on a concrete slab surface”
NRMCA says they run from about a quarter inch to 4 inches across, with a dense skin of mortar roughly an eighth of an inch thick sitting over a void. They can show up shortly after finishing, but in a dim garage or shop, small ones often go unnoticed until they break under traffic.
What delamination is
Delamination is the same problem on a bigger scale. From the companion bulletin, CIP 20, Delamination of Troweled Concrete Surfaces:
“Delaminations are separations of thin layers of the slab surface from the base concrete.”
They typically break off in layers an eighth to a quarter inch thick, and the bulletin says they can range from a few square inches to many square feet. In NRMCA’s words, “Delaminations are similar to blisters, but much larger”.
Here is the simple test you can do yourself:
“On a finished slab, delaminations can be detected by a hollow sound when tapped with a hammer or with a heavy chain drag.”
Tap the floor with a hammer every foot or so. Sound concrete rings solid. A delaminated area sounds dull and hollow. Mark the edges with chalk and you will have a map of the problem.
Why blisters and delamination happen
Both come from the same thing. Fresh concrete is still pushing air and bleed water up toward the top as it settles. If the surface gets sealed off before that air and water are out, they get trapped under a thin, dense crust. That crust is the blister, or the delaminated layer.
The surface usually gets sealed early for one of two reasons. Either the crew started troweling too soon, or the top of the slab stiffened faster than the concrete below it, so it looked ready when it was not. NRMCA’s advice to finishers:
“The finisher should be wary of a concrete surface that appears to be ready for final finishing before normally expected.”
And from the delamination bulletin:
“A slab without bleed water on the surface may not be ready to trowel.”
So what makes the top stiffen early? The bulletins list the usual causes, and several of them describe a normal day in Eastern Idaho.
1. Wind, sun and dry air. NRMCA lists high wind, low humidity, rising temperatures and direct sunlight as factors that stiffen the surface. Wind out here can dry the top of a slab in minutes while the inside is still soft.
2. A cold subgrade. When the ground under the slab is colder than the concrete, the top sets faster than the bottom. NRMCA calls this top-down stiffening. In our shoulder seasons, with frosty mornings and warm afternoons, that is a real risk. The delamination bulletin recommends avoiding placing concrete on a substrate colder than 40 degrees F, and the blister bulletin says that in cold weather the subgrade should be heated.
3. A vapor barrier right under the slab. Plastic under the slab means bleed water cannot drain down into the base, so more of it comes up, for longer. NRMCA lists placing a slab directly on a vapor retarder as a cause of both problems. That does not mean skip the vapor barrier on an interior floor that will get a covering. It is required there, and I covered why in my vapor barrier post. It means the crew has to respect the longer bleed time and not start finishing early.
4. Air entrainment on a troweled floor. Air-entrained concrete is the right call outside, for freeze-thaw durability. But it bleeds less and slower, so the surface can look ready too soon. NRMCA is direct about interior slabs:
“Air entrained concrete should not be specified for floor slabs that will receive a hard troweled finish as it increases the potential for delaminations.”
That is why the mix for a smooth troweled shop floor and the mix for a broom finished driveway are not the same order.
5. Overworking the surface. Excess vibration or too much floating works up a thick layer of mortar on top, which seals more easily. Tilting trowel blades too steeply on early passes does the same thing.
6. A sticky, overly rich mix. High cement or high fines content bleeds slower, which again makes the surface look ready before the concrete underneath is done.
How it gets prevented
These are straight from the NRMCA prevention lists, and they are the questions worth asking any crew pouring an interior floor.
- Do not seal the surface early. NRMCA’s first rule for avoiding delamination is not to over consolidate or seal the surface before air and bleed water have escaped.
- Check the set below the surface. A quarter inch boot print is the usual sign the slab is ready to trowel, and the bulletin suggests pushing a sharp object into the surface to make sure the concrete underneath is not still plastic.
- Keep the floats flat early. Flat blades on the first float pass so the surface stays open.
- Slow the surface drying, not the crew. On windy or hot days, NRMCA recommends covering with plastic or using evaporation retarders or fog sprays so the top does not crust over.
- Warm concrete in cold weather. Concrete over 50 degrees F with an accelerating admixture, so the slab sets evenly through its depth.
- Right mix for the finish. Non-air-entrained concrete for hard troweled interior floors, a slump in the 3 to 5 inch range, no extra water at the truck.
- Enough crew. NRMCA notes the crew size should be adequate for the area so parts of the slab are not finished too early just to keep up.
Can blisters and delamination be repaired?
Yes, but it is not quick. NRMCA says blisters “are not easily repaired after concrete hardens.” For delamination, the bulletin says:
“Delaminated surfaces can be repaired by patching after the surface layer is removed and the underlying concrete is properly cleaned.”
In practice that means mapping the hollow areas, cutting or chipping out the loose layer, cleaning down to sound concrete and patching with a proper repair material. When it is widespread, NRMCA says it may need grinding and a new overlay. If rusting steel near the surface caused it, the steel has to be cleaned too.
What does not work is gluing or sealing over a hollow layer. It will keep breaking off under traffic.
Frequently Asked Questions
What causes blisters on a new concrete slab?
Air or bleed water trapped under a surface that was sealed off too early by finishing, or a surface that stiffened faster than the concrete below it from wind, sun or a cold subgrade.
Why does my concrete floor sound hollow?
A hollow sound when you tap with a hammer usually means delamination, a thin layer of the surface separated from the concrete underneath. NRMCA describes hammer tapping and chain dragging as the standard way to find it.
Is a delaminated slab structurally unsafe?
Usually not. Finishing-related delamination is a surface layer problem, typically an eighth to a quarter inch thick. It is a durability and appearance issue, and it will keep breaking up under traffic until it is repaired.
Can you fix concrete blisters?
Small blisters caught during finishing can sometimes be worked back down. Once the concrete hardens, the loose skin has to be removed and patched, and larger areas may need grinding and an overlay.
Does a vapor barrier cause delamination?
A vapor barrier directly under the slab increases bleeding, which raises the risk if the crew finishes too early. It is still required under floors that will get a covering. The fix is patient finishing, not skipping the barrier.
Should my garage floor be air-entrained?
NRMCA recommends against air-entrained concrete for floors that get a hard troweled finish, because it increases the risk of delamination. Exterior flatwork exposed to freeze-thaw is a different case.
Floor sounding hollow?
If you are in Rigby, Idaho Falls, Rexburg, Ammon or Shelley and your slab has blisters, flaking or hollow spots, or you are planning a shop or garage floor and want it finished right, send me a few photos and I will tell you straight what you are dealing with.
Need concrete work in Eastern Idaho? Call Zach at Skinner Customs at (208) 390-5794 or start at skinner-customs.com.
Content produced in partnership with S4 Media, marketing partner of SwagerBuilds LLC.